A1 Vertaisarvioitu alkuperäisartikkeli tieteellisessä lehdessä
Silver diamine fluoride and resin-dentin bonding: Optimization of application protocols
Tekijät: Uctasli Merve, Stape Thiago Henrique Scarabello, Mutluay Mustafa Murat, Tezvergil-Mutluay Arzu
Kustantaja: Elsevier Ltd
Julkaisuvuosi: 2023
Journal: International Journal of Adhesion and Adhesives
Tietokannassa oleva lehden nimi: International Journal of Adhesion and Adhesives
Artikkelin numero: 103468
Vuosikerta: 126
ISSN: 0143-7496
eISSN: 1879-0127
DOI: https://doi.org/10.1016/j.ijadhadh.2023.103468
Verkko-osoite: https://doi.org/10.1016/j.ijadhadh.2023.103468
Rinnakkaistallenteen osoite: https://research.utu.fi/converis/portal/detail/Publication/180473958
Objective
To evaluate the effect of SDF-based treatments following delayed bonding and surface treatment approaches on resin-dentin bonding efficiency of a universal adhesive under different application modes.
Methods
Mid-coronal dentin surfaces from sound third molars were randomly treated with 38% silver diamine fluoride (SDF) and/or additionally with potassium iodide (SDF/KI). Untreated dentin served as control. SDF-treated teeth were assigned to groups according to surface treatment approaches (air-abrasion and water rinsing), the application mode of a mild universal adhesive (etch-and-rinse or self-etch) and delayed bonding (immediate, 7, 15 or 30 days). Microtensile bond strength (n = 5), SEM analyses of hybrid layer formation and dentin etching patterns and dentin permeability were evaluated. Data were analyzed with factorial ANOVA.
Results
SDF-based treatments affected dentin bonding depending on application mode and surface treatment approaches (p<0.001). Etch-and-rinse bonding was not affected by SDF-based treatments (p<0.05), producing more homogenous hybrid layers. While dentin etching patterns of etch-and-rinse application were not affected by SDF-based treatments, self-etching presented limitations. Bond strength reductions of self-etched dentin were restored by silver-removal strategies containing a water-rinsing step (p<0.05). Delayed bonding additionally reduced dentin permeability (p<0.05), further decreasing with longer periods (p<0.05).
Conclusion
Although the negative effect of SDF-based treatments on resin-dentin bonding can be avoided by strategies incorporating water-rinsing before hybridization, delayed bonding brings additional advantages due to higher mineral deposition.
Clinical significance
While the etch-and-rinse technique avoids major bonding drawbacks to SDF-treated dentin, self-etch bonding requires removal of excess silver deposits before hybridization. Performing SDF-based treatments and dentin hybridization in separate sessions (>15 days apart) potentialize mineral deposition improving caries control and service life of composite restorations.